Metal Alloys
Alloy Home
Steels
Alloy Steels
General Information
Properties
Classification
Standard
H-Steels
HSLA
Alloy Steel List
AISI 1xxx
AISI 2xxx
AISI 3xxx
AISI 4xxx
AISI 5xxx
AISI 6xxx
AISI 8xxx
AISI 9xxx
* For other AISI or Non-AISI, please use the search function above or check Grades.
ASTM Steels
Specific Alloy Steel
General Information
Resources
Bibliography
Negotiate Your Salary

Learn the best principles to negotiate the salary you deserve!

Mechanical Engineers Outlook

Guide for those interested in becoming a mechanical engineer. Includes qualifications, pay, and job duties.

CNC Machining Design Guide

Optimize your designs, reduce machining time, and lower your costs.

STEM Career Outlook

Wages, employment opportunities, and growth projections for STEM jobs.

more free publications
 
AISI 1330
Category Steel
Class Alloy steel
Type Standard
Common Names Manganese steel
Designations  Germany: DIN 1.1165
Japan: JIS SCMn 2 , JIS SMn 1 H
United States: ASTM A322 , ASTM A331 , ASTM A519 , MIL SPEC MIL-S-16974 , SAE J404 , SAE J412 , SAE J770 , UNS G13300

Composition

ElementWeight %
C  0.28-0.33 
Mn  1.60-1.90 
P  0.035 (max) 
S  0.04 (max) 
Si  0.15-0.30 

Mechanical Properties

Properties Conditions 
T (°C)Treatment
Density (×1000 kg/m3) 7.7-8.03 25  
Poisson's Ratio 0.27-0.30 25  
Elastic Modulus (GPa) 190-210 25  
Tensile Strength (Mpa) 1158  25  oil quenched, fine grained, tempered at 425°C  more
Yield Strength (Mpa) 1034 
Elongation (%) 15 
Reduction in Area (%) 53 
Hardness (HB) 335  25  oil quenched, fine grained, tempered at 425°C more
Glossary
Negotiate Your Salary

Learn the best principles to negotiate the salary you deserve!

Mechanical Engineers Outlook

Guide for those interested in becoming a mechanical engineer. Includes qualifications, pay, and job duties.

CNC Machining Design Guide

Optimize your designs, reduce machining time, and lower your costs.

STEM Career Outlook

Wages, employment opportunities, and growth projections for STEM jobs.