| Conditions | Tensile Properties |
| T (°C) | Treatment |
| 25 |
H1025 (bar, plate, sheet, strip) |
Tensile Strength (MPa) |
1070 |
| Yield Strength (MPa) |
1000 |
| Elongation (%) |
12 |
| Reduction in Area (%) |
45 |
| 25 |
H1075 (bar, plate, sheet, strip) |
Tensile Strength (MPa) |
1000 |
| Yield Strength (MPa) |
860 |
| Elongation (%) |
13 |
| Reduction in Area (%) |
45 |
| 25 |
H1100 (bar, plate, sheet, strip) |
Tensile Strength (MPa) |
965 |
| Yield Strength (MPa) |
795 |
| Elongation (%) |
14 |
| Reduction in Area (%) |
45 |
| 25 |
H1150 (bar, plate, sheet, strip) |
Tensile Strength (MPa) |
930 |
| Yield Strength (MPa) |
725 |
| Elongation (%) |
16 |
| Reduction in Area (%) |
50 |
| 25 |
H1150M (bar, plate, sheet, strip) |
Tensile Strength (MPa) |
795 |
| Yield Strength (MPa) |
515 |
| Elongation (%) |
18 |
| Reduction in Area (%) |
55 |
| 25 |
H900 (bar, plate, sheet, strip) |
Tensile Strength (MPa) |
1310 |
| Yield Strength (MPa) |
1170 |
| Elongation (%) |
10 |
| Reduction in Area (%) |
35 |
| 25 |
H925 (bar, plate, sheet, strip) |
Tensile Strength (MPa) |
11925 |
| Yield Strength (MPa) |
1070 |
| Elongation (%) |
10 |
| Reduction in Area (%) |
38 |