| AISI Type 405 | |
![]() | |
| Category | Steel |
| Class | Stainless steel |
| Type | Ferritic standard |
| Common Names | Chromium steel |
| Designations |
France: AFNOR Z 6 CA 13 Germany: DIN 1.4002 Italy: UNI X 6 CrAI 13 Japan: JIS SUS 405 United Kingdom: B.S. 405 S 17 United States: ASME SA240 , ASME SA268 , ASME SA479 , ASTM A176 , ASTM A240 , ASTM A268 , ASTM A276 , ASTM A314 , ASTM A473 , ASTM A479 , ASTM A511 , ASTM A580 , FED QQ-S-763 , MIL SPEC MIL.S-862 , SAE 51405 , SAE J405 (51405) , UNS S40500 |
| Composition | |
![]() | |
| Mechanical Properties | |
![]() | |
| Properties | Conditions | ||
| T (°C) | Treatment | ||
| Density (×1000 kg/m3) | 7.8 | 25 | |
| Poisson's Ratio | 0.27-0.30 | 25 | |
| Elastic Modulus (GPa) | 200 | 25 | |
| Tensile Strength (Mpa) | 480 | 25 | annealed, cold finished (plate, sheet, strip) more |
| Yield Strength (Mpa) | 275 | ||
| Elongation (%) | 16 | ||
| Reduction in Area (%) | 45 | ||
| Hardness (HRB) | 88 (max) | 25 | annealed (plate, sheet, strip) |
| Thermal Properties | |
![]() | |
| Properties | Conditions | ||
| T (°C) | Treatment | ||
| Thermal Expansion (10-6/ºC) | 10.8 | 0-100 more | |
| Thermal Conductivity (W/m-K) | 27 | 100 | |
| Specific Heat (J/kg-K) | 460 | 0-100 | |