| Ti-5Al-2.5Sn-ELI (low O2) | |
![]() | |
| Conditions | Tensile Properties | ||
| T (°C) | Treatment | ||
| -255 | annealed | Tensile Strength (MPa) | 1579 |
| Yield Strength (MPa) | 1420 | ||
| Elongation (%) | 15 | ||
| Reduction in Area (%) | |||
| -195 | annealed | Tensile Strength (MPa) | 1241 |
| Yield Strength (MPa) | 1158 | ||
| Elongation (%) | 16 | ||
| Reduction in Area (%) | |||
| 25 | annealed | Tensile Strength (MPa) | 807 |
| Yield Strength (MPa) | 745 | ||
| Elongation (%) | 16 | ||
| Reduction in Area (%) | |||