| Conditions | Tensile Properties |
| T (°C) | Treatment |
| 25 |
oil quenched, fine grained, tempered at 425°C |
Tensile Strength (MPa) |
1158 |
| Yield Strength (MPa) |
1034 |
| Elongation (%) |
15 |
| Reduction in Area (%) |
53 |
| 25 |
oil quenched, fine grained, tempered at 540°C |
Tensile Strength (MPa) |
876 |
| Yield Strength (MPa) |
772 |
| Elongation (%) |
18 |
| Reduction in Area (%) |
60 |
| 25 |
oil quenched, fine grained, tempered at 650°C |
Tensile Strength (MPa) |
731 |
| Yield Strength (MPa) |
572 |
| Elongation (%) |
23 |
| Reduction in Area (%) |
63 |
| 25 |
water quenched, fine grained, tempered at 205°C |
Tensile Strength (MPa) |
1600 |
| Yield Strength (MPa) |
1455 |
| Elongation (%) |
9 |
| Reduction in Area (%) |
39 |
| 25 |
water quenched, fine grained, tempered at 315°C |
Tensile Strength (MPa) |
1427 |
| Yield Strength (MPa) |
1282 |
| Elongation (%) |
9 |
| Reduction in Area (%) |
44 |