Metal Alloys
Alloy Home
Steels
Alloy Steels
General Information
Properties
Classification
Standard
H-Steels
HSLA
Alloy Steel List
AISI 1xxx
AISI 2xxx
AISI 3xxx
AISI 4xxx
AISI 5xxx
AISI 6xxx
AISI 8xxx
AISI 9xxx
* For other AISI or Non-AISI, please use the search function above or check Grades.
ASTM Steels
Specific Alloy Steel
General Information
Further Details
Resources
Bibliography
Selecting the Right 3D Printer

Discover how to choose the right 3D printer for your needs and the key performance attributes to consider.

Mechanical Engineers Outlook

Guide for those interested in becoming a mechanical engineer. Includes qualifications, pay, and job duties.

STEM Career Outlook

Wages, employment opportunities, and growth projections for STEM jobs.

Injection Molding Design Guide

Guide for high quality and cost-effective plastic injection molding.

more free publications
 
AISI 4037
Conditions Tensile Properties 
T (°C)Treatment
25 oil quenched, fine grained, tempered at 205°C   Tensile Strength (MPa) 1027 
Yield Strength (MPa) 758 
Elongation (%)
Reduction in Area (%) 38 
25 oil quenched, fine grained, tempered at 315°C   Tensile Strength (MPa) 951 
Yield Strength (MPa) 765 
Elongation (%) 14 
Reduction in Area (%) 53 
25 oil quenched, fine grained, tempered at 425°C   Tensile Strength (MPa) 876 
Yield Strength (MPa) 731 
Elongation (%) 20 
Reduction in Area (%) 60 
25 oil quenched, fine grained, tempered at 540°C   Tensile Strength (MPa) 793 
Yield Strength (MPa) 655 
Elongation (%) 23 
Reduction in Area (%) 63 
25 oil quenched, fine grained, tempered at 650°C   Tensile Strength (MPa) 696 
Yield Strength (MPa) 421 
Elongation (%) 29 
Reduction in Area (%) 60 
Glossary
Selecting the Right 3D Printer

Discover how to choose the right 3D printer for your needs and the key performance attributes to consider.

Mechanical Engineers Outlook

Guide for those interested in becoming a mechanical engineer. Includes qualifications, pay, and job duties.

STEM Career Outlook

Wages, employment opportunities, and growth projections for STEM jobs.

Injection Molding Design Guide

Guide for high quality and cost-effective plastic injection molding.