| Conditions | Tensile Properties |
| T (°C) | Treatment |
| 25 |
oil quenched, fine grained, tempered at 205°C |
Tensile Strength (MPa) |
1800 |
| Yield Strength (MPa) |
1662 |
| Elongation (%) |
12 |
| Reduction in Area (%) |
37 |
| 25 |
oil quenched, fine grained, tempered at 315°C |
Tensile Strength (MPa) |
1613 |
| Yield Strength (MPa) |
1455 |
| Elongation (%) |
13 |
| Reduction in Area (%) |
42 |
| 25 |
oil quenched, fine grained, tempered at 425°C |
Tensile Strength (MPa) |
1289 |
| Yield Strength (MPa) |
1172 |
| Elongation (%) |
15 |
| Reduction in Area (%) |
51 |
| 25 |
oil quenched, fine grained, tempered at 540°C |
Tensile Strength (MPa) |
986 |
| Yield Strength (MPa) |
883 |
| Elongation (%) |
20 |
| Reduction in Area (%) |
59 |
| 25 |
oil quenched, fine grained, tempered at 650°C |
Tensile Strength (MPa) |
793 |
| Yield Strength (MPa) |
689 |
| Elongation (%) |
28 |
| Reduction in Area (%) |
66 |