General Information
Further Details
Resources
Bibliography
CNC Machining Design Guide

Optimize your designs, reduce machining time, and lower your costs.

3D Scanners

A white paper to assist in the evaluation of 3D scanning hardware solutions.

STEM Career Outlook

Wages, employment opportunities, and growth projections for STEM jobs.

Mechanical Engineers Outlook

Guide for those interested in becoming a mechanical engineer. Includes qualifications, pay, and job duties.

more free publications
 
AISI 4140H
ConditionsHardness
T (°C)TreatmentMethodValue
25 annealed   HB 185-200 
25 annealed at 815°C   HB 197 
25 heat treated, oil-quenched, and tempered at 205°C   HB 520 
25 heat treated, oil-quenched, and tempered at 315°C   HB 455 
25 heat treated, oil-quenched, and tempered at 425°C   HB 385 
25 heat treated, oil-quenched, and tempered at 540°C   HB 320 
25 heat treated, oil-quenched, and tempered at 650°C   HB 255 
25 normalized at 870°C   HB 302 
25 normalized at 870°C, reheated to 845°C, quenched in oil, tempered at 205°C   HB 578 
25 normalized at 870°C, reheated to 845°C, quenched in oil, tempered at 260°C   HB 534 
25 normalized at 870°C, reheated to 845°C, quenched in oil, tempered at 315°C   HB 495 
25 normalized at 870°C, reheated to 845°C, quenched in oil, tempered at 370°C   HB 461 
25 normalized at 870°C, reheated to 845°C, quenched in oil, tempered at 425°C   HB 429 
25 normalized at 870°C, reheated to 845°C, quenched in oil, tempered at 480°C   HB 388 
25 normalized at 870°C, reheated to 845°C, quenched in oil, tempered at 540°C   HB 341 
25 normalized at 870°C, reheated to 845°C, quenched in oil, tempered at 595°C   HB 311 
25 normalized at 870°C, reheated to 845°C, quenched in oil, tempered at 650°C   HB 277 
25 normalized at 870°C, reheated to 845°C, quenched in oil, tempered at 705°C   HB 235 
Glossary
CNC Machining Design Guide

Optimize your designs, reduce machining time, and lower your costs.

3D Scanners

A white paper to assist in the evaluation of 3D scanning hardware solutions.

STEM Career Outlook

Wages, employment opportunities, and growth projections for STEM jobs.

Mechanical Engineers Outlook

Guide for those interested in becoming a mechanical engineer. Includes qualifications, pay, and job duties.