| AISI 5046 | |
![]() | |
| Conditions | Hardness | ||
| T (°C) | Treatment | Method | Value |
| 25 | oil quenched, fine grained, tempered at 205°C | HB | 482 |
| 25 | oil quenched, fine grained, tempered at 315°C | HB | 401 |
| 25 | oil quenched, fine grained, tempered at 425°C | HB | 336 |
| 25 | oil quenched, fine grained, tempered at 540°C | HB | 282 |
| 25 | oil quenched, fine grained, tempered at 650°C | HB | 235 |