| AA 1060 | |
![]() | |
| Conditions | Tensile Properties | ||
| T (°C) | Treatment | ||
| 25 | H12 | Tensile Strength (MPa) | 83 |
| Yield Strength (MPa) | 76 | ||
| Elongation (%) | 16 | ||
| Reduction in Area (%) | |||
| 25 | H14 | Tensile Strength (MPa) | 97 |
| Yield Strength (MPa) | 90 | ||
| Elongation (%) | 12 | ||
| Reduction in Area (%) | |||
| 25 | H16 | Tensile Strength (MPa) | 110 |
| Yield Strength (MPa) | 105 | ||
| Elongation (%) | 8 | ||
| Reduction in Area (%) | |||
| 25 | H18 | Tensile Strength (MPa) | 130 |
| Yield Strength (MPa) | 125 | ||
| Elongation (%) | 6 | ||
| Reduction in Area (%) | |||
| 25 | O | Tensile Strength (MPa) | 69 |
| Yield Strength (MPa) | 28 | ||
| Elongation (%) | 43 | ||
| Reduction in Area (%) | |||