295.0 | |
![]() | |


Conditions | Tensile Properties | ||
T (°C) | Treatment | ||
25 | T4 (sand casting) | Tensile Strength (MPa) | 220 |
Yield Strength (MPa) | 110 | ||
Elongation (%) | 8.5 | ||
Reduction in Area (%) | |||
25 | T6 (sand casting) | Tensile Strength (MPa) | 250 |
Yield Strength (MPa) | 165 | ||
Elongation (%) | 5.0 | ||
Reduction in Area (%) | |||
25 | T62 (sand casting) | Tensile Strength (MPa) | 285 |
Yield Strength (MPa) | 220 | ||
Elongation (%) | 2.0 | ||
Reduction in Area (%) |