| AA 5050 | |
![]() | |
| Conditions | Tensile Properties | ||
| T (°C) | Treatment | ||
| 25 | H32 | Tensile Strength (MPa) | 170 |
| Yield Strength (MPa) | 145 | ||
| Elongation (%) | 9 | ||
| Reduction in Area (%) | |||
| 25 | H34 | Tensile Strength (MPa) | 195 |
| Yield Strength (MPa) | 165 | ||
| Elongation (%) | 8 | ||
| Reduction in Area (%) | |||
| 25 | H36 | Tensile Strength (MPa) | 205 |
| Yield Strength (MPa) | 180 | ||
| Elongation (%) | 7 | ||
| Reduction in Area (%) | |||
| 25 | H38 | Tensile Strength (MPa) | 220 |
| Yield Strength (MPa) | 200 | ||
| Elongation (%) | 6 | ||
| Reduction in Area (%) | |||
| 25 | O | Tensile Strength (MPa) | 145 |
| Yield Strength (MPa) | 55 | ||
| Elongation (%) | 24 | ||
| Reduction in Area (%) | |||