| AA 5056 | |
![]() | |
| Category | Aluminum Alloy |
| Class | Wrought |
| Composition | |
![]() | |
| Mechanical Properties | |
![]() | |
| Properties | Conditions | ||
| T (°C) | Treatment | ||
| Density (×1000 kg/m3) | 2.64 | 25 | |
| Poisson's Ratio | 0.33 | 25 | |
| Elastic Modulus (GPa) | 70-80 | 25 | |
| Tensile Strength (Mpa) | 435 | 25 | H18 more |
| Yield Strength (Mpa) | 405 | ||
| Elongation (%) | |||
| Reduction in Area (%) | |||
| Hardness (HB500) | 105 | 25 | H18 more |
| Shear Strength (MPa) | 235 | 25 | H18 more |
| Fatigue Strength (MPa) | 150 | 25 | H18 more |
| Thermal Properties | |
![]() | |
| Properties | Conditions | ||
| T (°C) | Treatment | ||
| Thermal Expansion (10-6/ºC) | 24.1 | 20-100 | |
| Thermal Conductivity (W/m-K) | 112 | 25 | H38 more |
| Electric Properties | |
![]() | |