| AA 7075 | |
![]() | |
| Conditions | Tensile Properties | ||
| T (°C) | Treatment | ||
| 25 | O | Tensile Strength (MPa) | 230 |
| Yield Strength (MPa) | 105 | ||
| Elongation (%) | 17 | ||
| Reduction in Area (%) | |||
| 25 | O (Alclad) | Tensile Strength (MPa) | 220 |
| Yield Strength (MPa) | 95 | ||
| Elongation (%) | 17 | ||
| Reduction in Area (%) | |||
| 25 | T6 (Alclad) | Tensile Strength (MPa) | 525 |
| Yield Strength (MPa) | 460 | ||
| Elongation (%) | 11 | ||
| Reduction in Area (%) | |||
| 25 | T6 | Tensile Strength (MPa) | 570 |
| Yield Strength (MPa) | 505 | ||
| Elongation (%) | 11 | ||
| Reduction in Area (%) | |||
| 25 | T651 (Alclad) | Tensile Strength (MPa) | 525 |
| Yield Strength (MPa) | 460 | ||
| Elongation (%) | 11 | ||
| Reduction in Area (%) | |||
| 25 | T651 | Tensile Strength (MPa) | 570 |
| Yield Strength (MPa) | 505 | ||
| Elongation (%) | 11 | ||
| Reduction in Area (%) | |||
| 25 | T73 | Tensile Strength (MPa) | 505 |
| Yield Strength (MPa) | 435 | ||
| Elongation (%) | 13 | ||
| Reduction in Area (%) | |||