Metal Alloys
Alloy Home
Steels
Carbon Steels
General Information
Properties
Classification
Low-Carbon
Medium-Carbon
High-Carbon
Other Grades
Resulfurized
High-Mn
H-Steels
Carbon Steel List
AISI 10xx
AISI 11xx
AISI 12xx
AISI 15xx
ASTM Steels
Specific Carbon Stl.
General Information
Further Details
Resources
Bibliography
3D Scanners

A white paper to assist in the evaluation of 3D scanning hardware solutions.

Selecting the Right 3D Printer

Discover how to choose the right 3D printer for your needs and the key performance attributes to consider.

STEM Career Outlook

Wages, employment opportunities, and growth projections for STEM jobs.

Injection Molding Design Guide

Guide for high quality and cost-effective plastic injection molding.

more free publications
 
AISI 1006
Conditions Tensile Properties 
T (°C)Treatment
25 cold drawn (round bar (19-32 mm))  Tensile Strength (MPa) 330 
Yield Strength (MPa) 285 
Elongation (%) 20 
Reduction in Area (%) 45 
25 CQ,DQ and DQSK (sheet (1.6-5.8 mm))  Tensile Strength (MPa) 305-360
Yield Strength (MPa) 180-240
Elongation (%) 32-48 
Reduction in Area (%)  
25 hot rolled (round bar (19-32 mm))  Tensile Strength (MPa) 295 
Yield Strength (MPa) 165 
Elongation (%) 30 
Reduction in Area (%) 55 
Glossary
3D Scanners

A white paper to assist in the evaluation of 3D scanning hardware solutions.

Selecting the Right 3D Printer

Discover how to choose the right 3D printer for your needs and the key performance attributes to consider.

STEM Career Outlook

Wages, employment opportunities, and growth projections for STEM jobs.

Injection Molding Design Guide

Guide for high quality and cost-effective plastic injection molding.