AISI 1008 | |
![]() | |


Conditions | Tensile Properties | ||
T (°C) | Treatment | ||
25 | cold drawn (round bar (19-32 mm)) | Tensile Strength (MPa) | 340 |
Yield Strength (MPa) | 285 | ||
Elongation (%) | 20 | ||
Reduction in Area (%) | 45 | ||
25 | CQ,DQ and DQSK (sheet (1.6-5.8 mm)) | Tensile Strength (MPa) | 303-358 |
Yield Strength (MPa) | 180-240 | ||
Elongation (%) | 32-48 | ||
Reduction in Area (%) | |||
25 | hot rolled (round bar (19-32 mm)) | Tensile Strength (MPa) | 305 |
Yield Strength (MPa) | 170 | ||
Elongation (%) | 30 | ||
Reduction in Area (%) | 55 |