| AISI 1015 | |
![]() | |
| Conditions | Tensile Properties | ||
| T (°C) | Treatment | ||
| 25 | annealed at 870°C | Tensile Strength (MPa) | 386.1 |
| Yield Strength (MPa) | 284.4 | ||
| Elongation (%) | 37.0 | ||
| Reduction in Area (%) | 69.7 | ||
| 25 | normalized at 925°C | Tensile Strength (MPa) | 424.0 |
| Yield Strength (MPa) | 324.1 | ||
| Elongation (%) | 37.0 | ||
| Reduction in Area (%) | 69.6 | ||
| 25 | rolled | Tensile Strength (MPa) | 420.6 |
| Yield Strength (MPa) | 313.7 | ||
| Elongation (%) | 39.0 | ||
| Reduction in Area (%) | 61.0 | ||