AISI 1020 | |
![]() | |


Conditions | Tensile Properties | ||
T (°C) | Treatment | ||
25 | annealed at 870°C | Tensile Strength (MPa) | 394.7 |
Yield Strength (MPa) | 294.8 | ||
Elongation (%) | 36.5 | ||
Reduction in Area (%) | 66.0 | ||
25 | normalized at 870°C | Tensile Strength (MPa) | 441.3 |
Yield Strength (MPa) | 346.5 | ||
Elongation (%) | 35.8 | ||
Reduction in Area (%) | 67.9 | ||
25 | rolled | Tensile Strength (MPa) | 448.2 |
Yield Strength (MPa) | 330.9 | ||
Elongation (%) | 36.0 | ||
Reduction in Area (%) | 59.0 |