| AISI 1030 | |
![]() | |
| Category | Steel |
| Class | Carbon steel |
| Type | Standard |
| Designations |
Germany: DIN 1.1172 Italy: UNI CB 35 United States: ASTM A108 , ASTM A29 , ASTM A510 , ASTM A512 , ASTM A519 , ASTM A544 , ASTM A545 , ASTM A546 , ASTM A576 , ASTM A682 , FED QQ-S-635 (C1030) , FED QQ-S-700 (1030) , MIL SPEC MIL-S-11310 (CS1030) , SAE J403 , SAE J412 , SAE J414 , UNS G10300 |
| Composition | |
![]() | |
| Mechanical Properties | |
![]() | |
| Properties | Conditions | ||
| T (°C) | Treatment | ||
| Density (×1000 kg/m3) | 7.7-8.03 | 25 | |
| Poisson's Ratio | 0.27-0.30 | 25 | |
| Elastic Modulus (GPa) | 190-210 | 25 | |
| Tensile Strength (Mpa) | 463.7 | 25 | annealed at 845°C more |
| Yield Strength (Mpa) | 341.3 | ||
| Elongation (%) | 31.2 | ||
| Reduction in Area (%) | 57.9 | ||
| Hardness (HB) | 126 | 25 | annealed at 845°C more |
| Impact Strength (J) (Izod) |
69.4 | 25 | annealed at 845°C more |
| Thermal Properties | |
![]() | |