Metal Alloys
Alloy Home
Steels
Carbon Steels
General Information
Properties
Classification
Low-Carbon
Medium-Carbon
High-Carbon
Other Grades
Resulfurized
High-Mn
H-Steels
Carbon Steel List
AISI 10xx
AISI 11xx
AISI 12xx
AISI 15xx
ASTM Steels
Specific Carbon Stl.
General Information
Further Details
Resources
Bibliography
Desktop Engineering

Design, simulation, test, prototyping and high performance computing.

Essentials of Manufacturing

Information, coverage of important developments and expert commentary in manufacturing.

Salary Expectation

8 things to know about the interview question "What's your salary expectation"?

Negotiate Your Salary

Learn the best principles to negotiate the salary you deserve!

more free magazines
 
AISI 1040
ConditionsHardness
T (°C)TreatmentMethodValue
25 annealed at 790°C   HB 149 
25 normalized at 900°C   HB 170 
25 oil quenched, fine grained, tempered at 205°C   HB 262 
25 oil quenched, fine grained, tempered at 315°C   HB 255 
25 oil quenched, fine grained, tempered at 425°C   HB 241 
25 oil quenched, fine grained, tempered at 540°C   HB 212 
25 oil quenched, fine grained, tempered at 650°C   HB 192 
25 rolled   HB 201 
25 water quenched, fine grained, tempered at 205°C   HB 514 
25 water quenched, fine grained, tempered at 315°C   HB 444 
25 water quenched, fine grained, tempered at 425°C   HB 352 
25 water quenched, fine grained, tempered at 540°C   HB 269 
25 water quenched, fine grained, tempered at 650°C   HB 201 