Metal Alloys
Alloy Home
Steels
Carbon Steels
General Information
Properties
Classification
Low-Carbon
Medium-Carbon
High-Carbon
Other Grades
Resulfurized
High-Mn
H-Steels
Carbon Steel List
AISI 10xx
AISI 11xx
AISI 12xx
AISI 15xx
ASTM Steels
Specific Carbon Stl.
General Information
Resources
Bibliography
Metal 3D Printing Design Guide

Direct Metal Laser Sintering (DMLS) 3D printing for parts with reduced cost and little waste.

Selecting the Right 3D Printer

Discover how to choose the right 3D printer for your needs and the key performance attributes to consider.

CNC Machining Design Guide

Optimize your designs, reduce machining time, and lower your costs.

Negotiate Your Salary

Learn the best principles to negotiate the salary you deserve!

more free publications
 
AISI 1117
Category Steel
Class Carbon steel
Type Standard resulfurized
Designations  United States: AMS 5022G , ASTM A107 , ASTM A108 , FED QQ-S-637 (1117) , MIL SPEC MIL-S-18411 , SAE J403 , SAE J412 , SAE J414 , UNS G11170

Composition
ElementWeight %
C  0.14-0.20 
Mn  1.00-1.30 
P  0.04 (max) 
S  0.08-0.13 

Mechanical Properties
Properties Conditions 
T (°C)Treatment
Density (×1000 kg/m3) 7.7-8.03 25  
Poisson's Ratio 0.27-0.30 25  
Elastic Modulus (GPa) 190-210 25  
Tensile Strength (Mpa) 429.5  25  annealed at 855°C  more
Yield Strength (Mpa) 279.2 
Elongation (%) 32.8 
Reduction in Area (%) 58.0 
Hardness (HB) 121  25  annealed at 855°C more
Impact Strength (J)
(Izod)
93.6  25  annealed at 855°C  more
Glossary
Metal 3D Printing Design Guide

Direct Metal Laser Sintering (DMLS) 3D printing for parts with reduced cost and little waste.

Selecting the Right 3D Printer

Discover how to choose the right 3D printer for your needs and the key performance attributes to consider.

CNC Machining Design Guide

Optimize your designs, reduce machining time, and lower your costs.

Negotiate Your Salary

Learn the best principles to negotiate the salary you deserve!