| ASTM ZK21A-F | |
![]() | |
| Category | Magnesium Alloy |
| Composition | |
![]() | |
| Mechanical Properties | |
![]() | |
| Properties | Conditions | ||
| T (°C) | Treatment | ||
| Density (×1000 kg/m3) | 1.77-1.83 | 25 | |
| Poisson's Ratio | 0.35 | 25 | |
| Elastic Modulus (GPa) | 44.8 | 25 | |
| Tensile Strength (Mpa) | 260.0 | 25 | F (extruded bars and shapes) |
| Yield Strength (Mpa) | 195.0 (135.0) | ||
| Elongation (%) | 4.0 | ||
| Reduction in Area (%) | |||