Metal Alloys
Alloy Home
Steels
Stainless Steels
General Information
Properties
Stainless Stl. Grades
Austenitic
Martensitic
Ferritic
Precipitation Hardening
Stainless Steel List
AISI Type 2xx
AISI Type 3xx
AISI Type 4xx
AISI Type 5xx
AISI Type 6xx
* For other AISI or Non-AISI, please use the search function above or check Grades.
Specific Stainless Stl
General Information
Resources
Bibliography
STEM Career Outlook

Wages, employment opportunities, and growth projections for STEM jobs.

Metal 3D Printing Design Guide

Direct Metal Laser Sintering (DMLS) 3D printing for parts with reduced cost and little waste.

Mechanical Engineers Outlook

Guide for those interested in becoming a mechanical engineer. Includes qualifications, pay, and job duties.

Essentials of Manufacturing

Information, coverage of important developments and expert commentary in manufacturing.

more free publications
 
AISI Type 202
Category Steel
Class Stainless steel
Type Austenitic standard
Common Names Chromium-Manganese-Nickel steel
Designations  United States: ASTM A276 , ASTM A314 , ASTM A412 , ASTM A429 , ASTM A473 , ASTM A666 , FED QQ-S-763 , FED QQ-S-766 , FED STD-66 , SAE 30202 , SAE J405 (30202) , UNS S20200

Composition
ElementWeight %
C  0.15 
Mn  7.5-10.0 
Si  1.00 
Cr  17.0-19.0 
Ni  4.0-6.0 
P  0.06 
S  0.03 
N  0.25 

Mechanical Properties
Properties Conditions 
T (°C)Treatment
Density (×1000 kg/m3) 7.8 25  
Poisson's Ratio 0.27-0.30 25  
Elastic Modulus (GPa) 190-210 25  
Tensile Strength (Mpa) 515  25  annealed (sheet, strip) more
Yield Strength (Mpa) 275 
Elongation (%) 40 
Reduction in Area (%)  

Thermal Properties
Properties Conditions 
T (°C)Treatment
Thermal Expansion (10-6/ºC) 17.5  0-100 more  
Thermal Conductivity (W/m-K) 16.2  100 more  
Specific Heat (J/kg-K) 500  0-100   

Electric Properties
Properties Conditions 
T (°C)Treatment
Electric Resistivity (10-9W-m) 690  25   
Glossary
STEM Career Outlook

Wages, employment opportunities, and growth projections for STEM jobs.

Metal 3D Printing Design Guide

Direct Metal Laser Sintering (DMLS) 3D printing for parts with reduced cost and little waste.

Mechanical Engineers Outlook

Guide for those interested in becoming a mechanical engineer. Includes qualifications, pay, and job duties.

Essentials of Manufacturing

Information, coverage of important developments and expert commentary in manufacturing.