Metal Alloys
Alloy Home
Steels
Stainless Steels
General Information
Properties
Stainless Stl. Grades
Austenitic
Martensitic
Ferritic
Precipitation Hardening
Stainless Steel List
AISI Type 2xx
AISI Type 3xx
AISI Type 4xx
AISI Type 5xx
AISI Type 6xx
* For other AISI or Non-AISI, please use the search function above or check Grades.
Specific Stainless Stl
General Information
Resources
Bibliography
CNC Machining Design Guide

Optimize your designs, reduce machining time, and lower your costs.

STEM Career Outlook

Wages, employment opportunities, and growth projections for STEM jobs.

Mechanical Engineers Outlook

Guide for those interested in becoming a mechanical engineer. Includes qualifications, pay, and job duties.

Negotiate Your Salary

Learn the best principles to negotiate the salary you deserve!

more free publications
 
AISI Type 301
Category Steel
Class Stainless steel
Type Austenitic standard
Common Names Chromium-Nickel steel
Designations  France: AFNOR Z 12 CN 17.08
Germany: DIN 1.4310
Italy: UNI x 12 CrNi 17 07
Japan: JIS SUS 301
United States: AMS 5517 , AMS 5518 , AMS 5519 , ASTM A167 , ASTM A177 , ASTM A554 , ASTM A666 , FED QQ-S-766 , MIL SPEC MIL-S-5059 , SAE 30301 , SAE J405 (30301) , UNS 530100

Composition
ElementWeight %
C  0.15 
Mn  2.00 
Si  1.00 
Cr  16.0-18.0 
Ni  6.0-8.0 
P  0.045 
S  0.03 

Mechanical Properties
Properties Conditions 
T (°C)Treatment
Density (×1000 kg/m3) 8 25  
Poisson's Ratio 0.27-0.30 25  
Elastic Modulus (GPa) 193 25  
Tensile Strength (Mpa) 515  25  annealed (sheet, strip) more
Yield Strength (Mpa) 205 
Elongation (%) 40 
Reduction in Area (%)  
Hardness (HRB) 88 (max)  25  annealed (bar, wire, plate, sheet, strip) 

Thermal Properties
Properties Conditions 
T (°C)Treatment
Thermal Expansion (10-6/ºC) 17  0-100 more  
Thermal Conductivity (W/m-K) 16.2  100 more  
Specific Heat (J/kg-K) 500  0-100   

Electric Properties
Properties Conditions 
T (°C)Treatment
Electric Resistivity (10-9W-m) 720  25   
Glossary
CNC Machining Design Guide

Optimize your designs, reduce machining time, and lower your costs.

STEM Career Outlook

Wages, employment opportunities, and growth projections for STEM jobs.

Mechanical Engineers Outlook

Guide for those interested in becoming a mechanical engineer. Includes qualifications, pay, and job duties.

Negotiate Your Salary

Learn the best principles to negotiate the salary you deserve!