| AISI Type 301 | |
![]() | |
| Category | Steel |
| Class | Stainless steel |
| Type | Austenitic standard |
| Common Names | Chromium-Nickel steel |
| Designations |
France: AFNOR Z 12 CN 17.08 Germany: DIN 1.4310 Italy: UNI x 12 CrNi 17 07 Japan: JIS SUS 301 United States: AMS 5517 , AMS 5518 , AMS 5519 , ASTM A167 , ASTM A177 , ASTM A554 , ASTM A666 , FED QQ-S-766 , MIL SPEC MIL-S-5059 , SAE 30301 , SAE J405 (30301) , UNS 530100 |
| Composition | |
![]() | |
| Mechanical Properties | |
![]() | |
| Properties | Conditions | ||
| T (°C) | Treatment | ||
| Density (×1000 kg/m3) | 8 | 25 | |
| Poisson's Ratio | 0.27-0.30 | 25 | |
| Elastic Modulus (GPa) | 193 | 25 | |
| Tensile Strength (Mpa) | 515 | 25 | annealed (sheet, strip) more |
| Yield Strength (Mpa) | 205 | ||
| Elongation (%) | 40 | ||
| Reduction in Area (%) | |||
| Hardness (HRB) | 88 (max) | 25 | annealed (bar, wire, plate, sheet, strip) |
| Thermal Properties | |
![]() | |
| Properties | Conditions | ||
| T (°C) | Treatment | ||
| Thermal Expansion (10-6/ºC) | 17 | 0-100 more | |
| Thermal Conductivity (W/m-K) | 16.2 | 100 more | |
| Specific Heat (J/kg-K) | 500 | 0-100 | |
| Electric Properties | |
![]() | |