| AISI Type 305 | |
![]() | |
| Conditions | Tensile Properties | ||
| T (°C) | Treatment | ||
| 25 | annealed (plate, sheet, strip) | Tensile Strength (MPa) | 480 |
| Yield Strength (MPa) | 170 | ||
| Elongation (%) | 40 | ||
| Reduction in Area (%) | |||
| 25 | annealed (wire) | Tensile Strength (MPa) | 515 |
| Yield Strength (MPa) | 205 | ||
| Elongation (%) | |||
| Reduction in Area (%) | |||
| 25 | cold finished (wire) | Tensile Strength (MPa) | 620 |
| Yield Strength (MPa) | 310 | ||
| Elongation (%) | |||
| Reduction in Area (%) | |||
| 25 | cold finished and annealed (bar (up to 13 mm in diameter)) | Tensile Strength (MPa) | 260 |
| Yield Strength (MPa) | 310 | ||
| Elongation (%) | 30 | ||
| Reduction in Area (%) | 40 | ||
| 25 | cold finished and annealed (bar (over 13 mm in diameter)) | Tensile Strength (MPa) | 515 |
| Yield Strength (MPa) | 205 | ||
| Elongation (%) | 30 | ||
| Reduction in Area (%) | 40 | ||
| 25 | high tensile (bar, wire) | Tensile Strength (MPa) | 1690 |
| Yield Strength (MPa) | |||
| Elongation (%) | |||
| Reduction in Area (%) | |||
| 25 | hot finished and annealed (bar) | Tensile Strength (MPa) | 515 |
| Yield Strength (MPa) | 205 | ||
| Elongation (%) | 40 | ||
| Reduction in Area (%) | 50 | ||