| AISI L6 | |
![]() | |
| Conditions | Impact Energy (J) | ||
| T (°C) | Treatment | Method | Value |
| 25 | oil quenched from 845°C, single tempered at 315°C | Charpy V-notch | 12 |
| 25 | oil quenched from 845°C, single tempered at 425°C | Charpy V-notch | 18 |
| 25 | oil quenched from 845°C, single tempered at 540°C | Charpy V-notch | 23 |
| 25 | oil quenched from 845°C, single tempered at 650°C | Charpy V-notch | 81 |