| AISI S5 | |
![]() | |
| Conditions | Tensile Properties | ||
| T (°C) | Treatment | ||
| 25 | annealed | Tensile Strength (MPa) | 725 |
| Yield Strength (MPa) | 440 | ||
| Elongation (%) | 25 | ||
| Reduction in Area (%) | 50 | ||
| 25 | oil quenched from 870°C, single tempered at 205°C | Tensile Strength (MPa) | 2345 |
| Yield Strength (MPa) | 1930 | ||
| Elongation (%) | 5 | ||
| Reduction in Area (%) | 20 | ||
| 25 | oil quenched from 870°C, single tempered at 315°C | Tensile Strength (MPa) | 2240 |
| Yield Strength (MPa) | 1860 | ||
| Elongation (%) | 7 | ||
| Reduction in Area (%) | 24 | ||
| 25 | oil quenched from 870°C, single tempered at 425°C | Tensile Strength (MPa) | 1895 |
| Yield Strength (MPa) | 1690 | ||
| Elongation (%) | 9 | ||
| Reduction in Area (%) | 28 | ||
| 25 | oil quenched from 870°C, single tempered at 540°C | Tensile Strength (MPa) | 1520 |
| Yield Strength (MPa) | 1380 | ||
| Elongation (%) | 10 | ||
| Reduction in Area (%) | 30 | ||
| 25 | oil quenched from 870°C, single tempered at 650°C | Tensile Strength (MPa) | 1035 |
| Yield Strength (MPa) | 1170 | ||
| Elongation (%) | 15 | ||
| Reduction in Area (%) | 40 | ||