Metal Alloys
Alloy Home
Steels
Tool Steels
General Information
Properties
Tool Steel Types
High-Speed
Hot-Work
Cold-Work
Shock-Resistant
Mold
Special-Purpose
Water-Hardening
Tool Steel List
AISI Ax
AISI Dx
AISI Hx
AISI Lx
AISI Mx
AISI Ox
AISI Px
AISI Sx
AISI Tx
AISI Wx
Resources
Bibliography
Essentials of Manufacturing

Information, coverage of important developments and expert commentary in manufacturing.

Chemical Engineering

The industry gateway for chemical engineering and plant operations.

NASA Tech Briefs

Innovations developed by NASA and its industry partners in a wide array of fields.

Laser Focus World

Semiconductors, medical equipment, lasers, optics and aviation and aerospace.

more free magazines
 
AISI T1
Category Steel
Class Tool steel
Type Tungsten high speed steel
Designations  France: AFNOR 18-04-01
Germany: DIN 1.3355
Italy: UNI X 75 W 18 KU
Japan: JIS SKH2
United Kingdom: B.S. BT 1
United States: AMS 5626 , ASTM A600 , FED QQ-T-590 , SAE J437 , SAE J438

Composition
ElementWeight %
C  0.65-0.80 
Mn  0.10-0.40 
Si  0.20-0.40 
Cr  3.75-4.00 
Ni  0.3 
W  17.25-18.75 
V  0.90-1.30 
Cu  0.25 
P  0.03 
S  0.03 

Mechanical Properties
Properties Conditions 
T (°C)Treatment
Density (×1000 kg/m3) 8.67 25  
Poisson's Ratio 0.27-0.30 25  
Elastic Modulus (GPa) 190-210 25  

Thermal Properties
Properties Conditions 
T (°C)Treatment
Thermal Expansion (10-6/ºC) 9.7  20-200 more  
Thermal Conductivity (W/m-K) 19.9  100 more  